Techsil TIM11150 (GB)

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

Techsil TIM11150 (GB)20oz

Main features

  • 2.30 W/(m K) Thermal Conductivity
  • Embedded 50 um Glass Beads
  • Non-Corrosive Bonding Formulation

Product Description

Techsil® TIM11150 (GB) is a one-part, solvent-free acetone-cure RTV silicone sealant containing 50 µm glass beads for controlled self-gapping applications. The grey paste cures through atmospheric moisture to form a tough elastomer and is non-corrosive to copper and copper alloys. It combines fast skin formation with a typical cured thermal conductivity of 2.30 W/m·K and documented electrical insulation properties.

Key features

  • Thermally conductive cured elastomer: Provides a typical thermal conductivity of 2.30 W/m·K after seven days of cure at 23 ± 2 °C and 65% relative humidity.
  • Controlled self-gapping: Contains 50 µm glass beads to maintain separation in supported self-gapping applications.
  • Non-corrosive moisture cure: The one-part, solvent-free acetone-cure system does not corrode copper or copper alloys and reaches tack-free condition in four minutes under stated conditions.

Applications / Suitable for

  • Self-gapping applications requiring 50 µm glass-bead spacing
  • Sealing and adhesive applications where a one-part RTV silicone is suitable
  • Applications involving copper or copper-alloy surfaces where non-corrosive cure is required
Product Family

TECHSIL TIM11150GB

Catalog Product

Unlike other products we offer, the products listed on this page cannot currently be ordered directly from the website.

TDS, SDS & Technical Documents

Technical Specifications

General Properties
AppearanceAppearance
gray paste
ColorColor
gray
Specific GravitySpecific Gravity
2.11
Physical Properties
Tack-Free TimeTack-Free Time
4 minutes
ViscosityViscosity
350,000 mPa.s
Mechanical Properties
ElongationElongation
103 %
Thermal Properties
Operating TemperatureOperating Temperature
-50 to 220 °C
Thermal ConductivityThermal Conductivity
2.30 W/m.K

Additional Information

Technical properties

As-supplied / before-processing properties

Typical uncured and processing properties of Techsil® TIM11150 (GB). Typical technical data are not intended for specification purposes.

Property Value Unit Method / condition
Chemistry and cure type One-part, acetone-cure RTV silicone — Moisture cure; solvent free
Color and appearance Grey paste — As supplied
Glass-bead particle size 50 µm For self-gapping applications
Viscosity 350,000 mPa·s Brookfield
Tack-free time 4 minutes Measured at 23 ± 2 °C and 65% relative humidity
Cure-through time <8 hours 3 mm section at 23 ± 2 °C and 65% relative humidity
Full cure 7 days Supplier-stated full-cure time
Shelf life 12 months Expected in original unopened containers stored below 40 °C
Technical properties

After-processing / final-state properties

Typical cured properties of Techsil® TIM11150 (GB) after seven days at 23 ± 2 °C and 65% relative humidity, except where otherwise stated. Typical technical data are not intended for specification purposes.

Property Value Unit Method / condition
Tensile strength 3.90 MPa BS 903 Part A2
Elongation at break 103 % BS 903 Part A2
Hardness 67 Shore A ASTM D2240-95
Specific gravity 2.11 — BS 903 Part A1
Linear shrinkage 0.5 % Test method not stated
Thermal conductivity 2.30 W/m·K Test method not stated
Service temperature -50 to 220 °C Minimum stated without method; maximum per AFS 1540B
Volume resistivity 1 × 1014 Ω·cm ASTM D257
Dielectric strength 20 kV/mm ASTM D149

Leading Brands Trust in Our Products and Services

  • Jabil
  • Linxens
  • Magna
  • Medtronic
  • NXP
  • Philips
  • Semikron
  • Teledyne
  • Thales
  • Vishay
  • ZF
  • AMS
  • Apple
  • Audi
  • Broadcom
  • Borgwarner
  • Bosch
  • Eaton
  • Henkel
  • Honeywell
  • Hysol
  • Intel
Products that Perform|Knowledge that Serves|Service that Delivers